I was asked to make a friend some drawer pulls and cabinet handles. How do I embed the machine screws into the piece so the screw doesn't crack the handle as it dries?

Share this post


Link to post
Share on other sites
Mark C.    1,797

Clay shrinks and will crack with the screw left in

How about using a metal screw insert in the pull. Make an oversize hole that will fit insert when fired (shrinks 12% or less)then epoxy insert into pull and screw into insert.

If you want the screw than ream out the screw hole a bunch and let shrink without screw-fire and hope it fits then-I would do the insert hole and glue.

Mark

Share this post


Link to post
Share on other sites
TJR    359

Mark is correct. Don't fire the screws in the kiln. Make a hollow in the back of your pull so that you can cement the screw in after firing.

TJR.

Share this post


Link to post
Share on other sites
neilestrick    1,379

 

HERE. A brass insert is glued in after firing. Drill the hole when leather hard, just slightly deeper than you'll need. You'll have to calculate for shrinkage to see what size drill bit to use.

Share this post


Link to post
Share on other sites
AtomicAxe    19

What mark said. slightly bigger hole than threaded pole, when fired ... epoxy in. Threaded shafts are easy to find .. just make sure you get nuts and washers to go with them at the same time so it's a match and a simple matter.

Share this post


Link to post
Share on other sites
Pres    896

I fixed the link above.

 

 

I did pulls years ago, and instead of regular epoxy I used the plumbers type epoxy putty. It has a little more body, and can be filed or tooled afterwards.

Share this post


Link to post
Share on other sites
neilestrick    1,379

I used epoxy putty for a while, but found it to be a bit awkward and messy, and required too much tooling and cleanup. The last batch I did with regular 2 part epoxy in the tubes. I found that if the hole was about 1/16 inch deeper than the plug, and just a hair wider, like almost no wiggle, I could put a big drop of epoxy in the hole, slide in the plug and it would squeeze just enough glue up the sides to hold it perfectly without any oozing out. Did a batch of 20 in just a couple minutes. I mark my drill bit depth with a piece of tape when making the holes.

Share this post


Link to post
Share on other sites
Tikiguy    1

post-32000-136735719965_thumb.jpgThis is the original sculpture for the pulls. I just finished prepping it for making a mold. when finished it'll have a short bamboo tube that carries it to the cabinet door. Sorry... I shot the photo with my Ipod, a little fuzzy.

Thank you all for your help.

Share this post


Link to post
Share on other sites
Pres    896

I used epoxy putty for a while, but found it to be a bit awkward and messy, and required too much tooling and cleanup. The last batch I did with regular 2 part epoxy in the tubes. I found that if the hole was about 1/16 inch deeper than the plug, and just a hair wider, like almost no wiggle, I could put a big drop of epoxy in the hole, slide in the plug and it would squeeze just enough glue up the sides to hold it perfectly without any oozing out. Did a batch of 20 in just a couple minutes. I mark my drill bit depth with a piece of tape when making the holes.

 

never had much of a problem with mess. Roll out a coil thinner than hole, ram in the screw, compact the top edge with old credit card. File when dry. Different strokes for different folks.

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now
Sign in to follow this  

×