Recommended Posts

I recently got a used electric kiln which I've been glaze firing to cone 5/6. The person who had it previously only fired low fire. I am noticing that the shelves are warping and i plan to wash the other sides and turn them over each time I fire from now on. My question is: are the shelves perhaps not rated to go to mid range? Should I eventually get new shelves? The kiln I fire where I teach has very old shelves that aren't warped at all...are they made for higher temps.?

Thanks!

Link to comment
Share on other sites

I recently got a used electric kiln which I've been glaze firing to cone 5/6. The person who had it previously only fired low fire. I am noticing that the shelves are warping and i plan to wash the other sides and turn them over each time I fire from now on. My question is: are the shelves perhaps not rated to go to mid range? Should I eventually get new shelves? The kiln I fire where I teach has very old shelves that aren't warped at all...are they made for higher temps.?

Thanks!

 

 

If they are half inch "clay" (corderite/alumina/some variation thereof) they really dont last at cone 6. You have to use a thicker shelf or a thin SiC shelf, if you can justify the cost.

Link to comment
Share on other sites

I've heard nothing but good things about hollow core shelves- CoreLite. Light and strong, and no more expensive than standard cordierite shelves. I got a few 14x28 recently, and they've held up well so far.

 

 

I knew someone recently who got a bad batch of those Corelite shelves, they were the largest they make for a round top-loader. Every single one cracked nicely down the middle--I saw her stack and posting--so did Resco the mfr). Resco insisted that it wasn't a manufacturing issue, but they were also completely happy to refund her $$$. I have encountered other folks with similar issues (but only with the very largest of shelves) and a tech @ Resco spoke to acknowledged that at one point they had issues with the extrusions being prone to cracking due to a an issue with either the die or the method by which they were cutting them, I forget. Either way he said it was resolved, but I sort of wonder.

Link to comment
Share on other sites

I've heard nothing but good things about hollow core shelves- CoreLite. Light and strong, and no more expensive than standard cordierite shelves. I got a few 14x28 recently, and they've held up well so far.

 

 

I knew someone recently who got a bad batch of those Corelite shelves, they were the largest they make for a round top-loader. Every single one cracked nicely down the middle--I saw her stack and posting--so did Resco the mfr). Resco insisted that it wasn't a manufacturing issue, but they were also completely happy to refund her $$. I have encountered other folks with similar issues (but only with the very largest of shelves) and a tech @ Resco spoke to acknowledged that at one point they had issues with the extrusions being prone to cracking due to a an issue with either the die or the method by which they were cutting them, I forget. Either way he said it was resolved, but I sort of wonder.

 

 

Interesting. Hopefully it truly is worked out. I tend to give them the benefit of the doubt, because if they didn't fix it word would get out quickly if the problem persisted. They HAVE to fix it to stay in business. The folks at Lill Street have been using them in their gas kilns for the last few years and they still haven't warped. Seems like every brand goes through some issues at some point. Thorley's went bad when Laguna first bought them out, but they got it figured out.

Link to comment
Share on other sites

  • 4 months later...

I've heard nothing but good things about hollow core shelves- CoreLite. Light and strong, and no more expensive than standard cordierite shelves. I got a few 14x28 recently, and they've held up well so far.

 

 

 

I had one 21" crack clear across the middle first cone 6 firing, Standard Ceramic replaced it. After about a year, many 06 and just a few 6 firings two more just cracked clear across the middle on a 6 firing. They're light for a deep top loader, but I'm sure reluctant to try them again.

Link to comment
Share on other sites

  • 1 year later...

I flip them about every other firing. Since I have a supply of the older 1 in shelves, I use the light weight ones higher in the kiln where it's hard to lift the others head high, getting too old and too slow to play like I was 50 :)

Higher is also a 1/2 cone cooler.

Wyndham

Link to comment
Share on other sites

Archived

This topic is now archived and is closed to further replies.

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.