preparing raw majolica glaze for surface decoration.

Recommended Posts

Babs    386

Hi I am looking for a way to make my raw majolica glaze "harder" so that I can ddo more painterly desings on my ware. Mybrush tends to clog up with the glaze powder and so the lines are interrupted.

Hope somepone can help. I think I readd somewhere that you can spray something onto the glaze.Does any one have any hints.

Babs

Share this post


Link to post
Share on other sites
Iforgot    2

You can fire your ware to cone 018 after you glaze and sand the peice. This cinters the glaze paricles making it a bit more sturdy.

 

 

 

 

 

Darrel

Share this post


Link to post
Share on other sites
Babs    386

Thanks everyone for your practical suggestions as I was dreading having to rejig my glaze recipe for this order, someone wanting handwritten text on some posts..

Babs

Share this post


Link to post
Share on other sites
Marcia Selsor    1,301

As previously mentioned you can spray it with spray starch or cheap hair spray. You can also add a little liquid starch into the glaze batch.

I think it is mentioned in Arbuckle's information.

 

Marcia

Share this post


Link to post
Share on other sites
perkolator    53

add CMC to your base glaze. commercial glazes contain a good amount of this in their recipe. it forms sort of a "candy coating" and stiffens up the unfired glaze, which will be more resistant to your detail brush. start with around 1% or keep a thick solution of it in a jug to add to your glazes, underglazes, and stains/washes.

Share this post


Link to post
Share on other sites
Babs    386

Thanks everyone, about to bisque the 'thing' and then pending survival, will glaze and decorate using your suggestions.

Thanks again.

Babs

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now
Sign in to follow this  

×