Handle attachment crack...patch before bisquing?

Recommended Posts

Ginny C    5

If I succeed in uploading a photo, you'll see a crack where the handle attaches to a bone dry mug. The crack doesn't go all the way around, just across the top half. (I know it's because the cup was a bit too dry when I attached the handle, but I'd like to save it if possible! I dried it upside down so the weight wouldn't pull the handle off, but this crack appeared anyway.)

Should I brush in some paper clay slip? I have some that's pretty thick and stiff, so it wouldn't add much moisture.

 

If I don't, is the crack likely to get worse in the bisque firing??

 

Laguna B-mix cone 5. Will bisque to 06 and then glaze fire to cone 6.

 

Ginny C

post-1066-135863445281_thumb.jpg

post-1066-135863445281_thumb.jpg

Share this post


Link to post
Share on other sites
Mark C.    1,797

Best fixed before bisquing-Tool in some slip and then after drying rub it out with a sharp tool. Then fire.If its still cracked after firing try some bisque fix by amaco.

Mark

Share this post


Link to post
Share on other sites
Mark C.    1,797

You can use a kiln cement on the crack after bisquing to get the strength back.Hi fire mender is one I like as you mix your clay body with it and then mix it so repairs are a good match.

Mark

Share this post


Link to post
Share on other sites
emptynester    2

I can see why you would like to save it. It has nice details. That being said, I would reclaim the clay now. I haven't had great results with repairs. The glaze seems to high light the repaired area.

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now
Sign in to follow this  

×