Posted 19 January 2013 - 05:29 PM

If I succeed in uploading a photo, you'll see a crack where the handle attaches to a bone dry mug. The crack doesn't go all the way around, just across the top half. (I know it's because the cup was a bit too dry when I attached the handle, but I'd like to save it if possible! I dried it upside down so the weight wouldn't pull the handle off, but this crack appeared anyway.)
Should I brush in some paper clay slip? I have some that's pretty thick and stiff, so it wouldn't add much moisture.

If I don't, is the crack likely to get worse in the bisque firing??

Laguna B-mix cone 5. Will bisque to 06 and then glaze fire to cone 6.

Ginny C
Attached File  IMG_6643.jpg   994.84KB   103 downloads

#2 Mark C.

Mark C.

    Advanced Member

  • Members
  • PipPipPip
  • 6,378 posts
  • LocationNear Arcata Ca-redwood rain forest

Posted 19 January 2013 - 05:32 PM

Best fixed before bisquing-Tool in some slip and then after drying rub it out with a sharp tool. Then fire.If its still cracked after firing try some bisque fix by amaco.
Mark
Mark Cortright
www.liscomhillpottery.com

#3 Chris Campbell

Chris Campbell

    clay stained since 1988

  • Members
  • PipPipPip
  • 3,137 posts
  • LocationRaleigh, NC

Posted 19 January 2013 - 05:45 PM

Just be very aware of that mug if you try to use it for hot beverages as that might always be a weak spot. Cracks never really go away. : - )
Chris Campbell Pottery
Contemporary Fine Colored Porcelain
http://ccpottery.com/

>TRY ... FAIL ... LEARN ... REPEAT"

" If a sufficient number of people are different, no one has to be normal "

Fredrick Bachman

#4 Mark C.

Mark C.

    Advanced Member

  • Members
  • PipPipPip
  • 6,378 posts
  • LocationNear Arcata Ca-redwood rain forest

Posted 19 January 2013 - 09:36 PM

You can use a kiln cement on the crack after bisquing to get the strength back.Hi fire mender is one I like as you mix your clay body with it and then mix it so repairs are a good match.
Mark
Mark Cortright
www.liscomhillpottery.com

#5 OffCenter

OffCenter

    Advanced Member

  • Members
  • PipPipPip
  • 1,372 posts

Posted 19 January 2013 - 10:27 PM

Toss it or you'll spend more time "fixing" it (and not being sure it's really fixed) than it would take to make a replacement.

Jim
E pur si muove.

"But it does move," said Galileo under his breath.

#6 JessicaGrayCeramics

JessicaGrayCeramics

    Member

  • Members
  • PipPip
  • 12 posts
  • LocationFeltwell, United Kingdom

Posted 20 January 2013 - 05:43 AM

Toss it or you'll spend more time "fixing" it (and not being sure it's really fixed) than it would take to make a replacement.


I'm with Jim. At least at this point, you can still reuse the clay.
Jessica Gray, MFA
www.JessicaGrayCeramics.com

#7 emptynester

emptynester

    Member

  • Members
  • PipPip
  • 15 posts

Posted 20 January 2013 - 10:00 AM

I can see why you would like to save it. It has nice details. That being said, I would reclaim the clay now. I haven't had great results with repairs. The glaze seems to high light the repaired area.

#8 Iforgot

Iforgot

    Advanced Member

  • Members
  • PipPipPip
  • 155 posts
  • LocationColorado

Posted 20 January 2013 - 12:57 PM

I'd shove some sodium sillicate into the crack with a hard brush before bisque.