mudpups Posted December 11, 2012 Report Share Posted December 11, 2012 I found a thread about this where someone gave a recipe - something like; 1 part stain, 1 part frit, 1 part bentonite. I kept the page open, went out to walk the dog, came back to get the recipe to make it and my computer had crashed - do you think i can find that thread again! NO! Please, what was the recipe to turn a stain into an underglaze? Link to comment Share on other sites More sharing options...
Marcia Selsor Posted December 11, 2012 Report Share Posted December 11, 2012 This is a recipe for low fire ^04 underglaze stain from Val Cushing. By weight: 25 ep kaolin 25 frit 3110 25 stain....you can vary the stain for intensity. 25 or 1/3 is pretty intense. This is mostly using for highlighting textured surfaces. Marcia Link to comment Share on other sites More sharing options...