Best i can tell, it looks like a clear or a semi opaque white glaze over a dark body, with heavy iron grog causing the speckling.

 

I will sometimes add a 50/50 mix of dark (iron rich) silica sand and high iron grog to a white stoneware body yielding a nice white background with plenty or flecking. the raw clay has a sort of "cookies n' cream" candy bar look.

 

Or adding granular magnetite or ilmenite can give similar effects when added to your favourite clear or white glaze. Pitting and uneven/ hard to control flecking can also occur.

 

Firing in reduction will enhance the flecking/speckling from the clay body.

 

-Burt

Share this post


Link to post
Share on other sites

Huh. upon a little googling....... Ishihaze is in reference to small stones in the clay expanding in the firing and sticking out into the glaze layer.....

 

IDK anything about this!

 

But it sure sounds like a big old hunk of heavy iron grog, maybe even use kyanite like in Soldners Raku body.

 

-Burt

Share this post


Link to post
Share on other sites

looks like it's in part - in the clay.

 

Ishihaze. A "stone explosion." Before firing, many of the impurities of the clay are removed. But some potters like rougher clay, and leave in small stones that sometimes burst out on the surface during firing - called ishihaze. Often found on Bizen and other yakishime (high-fired unglazed stonewares). http://www.e-yakimono.net/guide/html/techniques.html

Share this post


Link to post
Share on other sites

Thank you all for the speedy reply and information.

 

A video called Japanese Pottery History said there is Potash and iron in the clay body, so maybe that's it.

 

I was about to ask can you add GROG to the glaze or the clay to create this effect and the answers below suggested this.

 

What is it like round2potter to throw with the grog clay? I just bought some fine grog today, but it doesn't look so fine to me and i'm wondering how to make it finer.

 

I wonder if I can make a billyjoesbutterwhite by adding some iron to the body? Or Mark, do you know where to find the recipe please? Or would iron shavings from a bbq scourer do the trick? How much exactly would I need to use?

 

And is it food safe with so much iron in the clay?

Edited by Essaily

Share this post


Link to post
Share on other sites

Hmmmm foodsafe....probably, and i am sure somebody will jump on me for this but at worst your just getting your diet fortified with a little iron, just like they put iron in corn flakes.

 

Food safety depends on the glaze and the clay, and the firing schedule.

 

I LOVE TO THROW WITH GROGGY CLAY!!!

 

A lot of people i have worked with complain that the groggy clay i use tears up their hands.

As a result my hands are always baby smooth.

 

But it all depends on what you are doing with it, and just how big the grog is. I don't really use much anything bigger than sand size pieces; half of what I add to the white stoneware (which has fine grog) is sand.

 

Only once has grog drawn blood for me; and I was removing the excess clay at the skirt of a pot with my finger. The pressure onto the wheelhead caused a hunk to sink itself in the pad of my finger.

 

I do however use fine grog in my clay,

 

The added strength is amazing, and i am fairly certain it helps the clay to withstand thermal shock

 

Also, heavy grog will catch and drag on a trimming tool; its not a problem really, but some would say a fine grogged body is easier to trim.

 

-Burt

Share this post


Link to post
Share on other sites
Guest JBaymore

Ishihaze effects are caused by small bits of granular feldspathic rocks and quartz rocks in the clay body. It comes from the Japanese 石爆ãœ.  石 = ishi = stone 爆㜠= haze = burst open

 

For the "premier" examples of this effect, research the ceramics made in the town of Shigaraki in Shiga Prefecture. The best clay for this in Shigaraki is called Kinose. The deposits of the best clay are severely depleted... and if you can get it.... it is very expensive stuff.

 

One interesting technique (not from Shigaraki) is to put a layer of a high kaolin white slip in a thin coating over the clay body containing the rocks. Then the rocks sort of break through the slip layer as the clay shrinks in the firing. Over this is a layer of a milky transparenty glaze.

 

If you want a US commercially prepared clay that is somewhat like this kind of Shigaraki Nasty Clay thing, get "Grogzilla" from Clay Planet )Orton Cone 9-10 clay).

 

 

 

The images you posted look more like just the effect of hematite (iron) nodules in the clay body bleeding into the glaze layer rather than "ishihaze". But it might be the resolution of the pictures so I can't see it.

 

best,

 

 

............john

Share this post


Link to post
Share on other sites

I'll second the Grogzilla if you want freaky things popping through your glaze from the clay! This was fired to cone 5 (Clay planet lists this as a cone 5-10 clay, so you know its not really vitrified at cone 5) with a brick red glaze over it. The glaze has a bit of dark speckle, but the white flecks in this are from the clay. I did wipe the surface on the greenware back with a damp sponge to make it rougher, I was going for a thang with this one smile.gif

 

post-14098-135539009207_thumb.jpg

 

Anyway, Grogzilla is crazy groggy, some of the grog is almost 1/8th of an inch so its probably not great for wheelwork. Works fine handbuilding though!

post-14098-135539009207_thumb.jpg

Share this post


Link to post
Share on other sites

I can see the pitting in your red glaze, Weeble - really like that look, like a rock surface! I watched the video again just now, to find out why I like it so much, I don't know, I think its so humble looking with no trace of the maker except for the uneven throwing and understated glaze - that's the reason. Is it food safe btw, with all those pits and bubbles? Thanks for the name of the clay. Not sure we have it in Oz. Shall make my own.

Share this post


Link to post
Share on other sites

Ehhh, I wouldn't use Grogzilla for food, not the way I used it anyway, because its so porous at cone 5. Even for the bonsai pots I'm a bit leery, its really a sculptural clay. This was a one-off, I was trying to use the last of a brick and demo a technique for a student. It'll absorb a lot of moisture and I expect a fairly short life span on this pot, especially if someone leaves it out to run through freeze/thaw cycles. The thing the Grogzilla does that I've not seen in other prepared clays is it throws out little white lumps in the firing. Most of those 'pits' you are seeing are actual little bumps of white material that sticks up through the surface of the glaze.

 

A technique I've used for pitted surfaces with hand-building is to roll cornmeal or coffee grounds or some other organic material into the surface then burnish it in. It burns out in the firing, leaving a bunch of small pits that are pretty cool.

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now
Sign in to follow this  

×

Important Information

By using this site, you agree to our Terms of Use.