I’m an amateur, and it shows.


  • Please log in to reply
5 replies to this topic

#1 socaljim

socaljim

    Newbie

  • Members
  • Pip
  • 2 posts

Posted 08 December 2012 - 12:53 AM

I was hoping someone would be ableto give me some advice. I usually only use my kiln for green ware firing andglazing. This was my first attempt at over-glaze. I fired my bisque to cone 04and glazed it with gloss glaze to cone 06. I bought a bottle of Colorobbia goldand the clerk told me to brush it on and fire to cone 018. I think I missedsomething. I’m not sure if I didn’t apply enough, I applied to much, the conewas too hot / too cold, or the gloss glaze was the wrong type. What did I dowrong? Also, if anyone can tell me how I can fix the 30 pieces that I ruined itwould be greatly appreciated. Please see attached pictured.

Attached Files

  • Attached File  gold.JPG   376.61KB   133 downloads


#2 Marcia Selsor

Marcia Selsor

    Professor Emerita, MSU-Billings

  • Members
  • PipPipPip
  • 5,438 posts
  • LocationBrownsville, Texas

Posted 08 December 2012 - 09:25 AM

I have not done this in a while but I always fired with the lid slightly open when doing lusters. My gold luster bottle says 019.
SO maybe you did go slightly hotter than recommended. Did you have the lid closed? If your kiln is vented, this may not be necessary.

Lusters really stink. They are very toxic. You need good ventilation and better yet, don't be near the kiln room when firing.

Marcia



Marcia Selsor, Professor Emerita,
Montana State University-Billings

Marcia Selsor Studio in Brownsville, Texas.

http://www.marciaselsorstudio.com


#3 Lucille Oka

Lucille Oka

    Advanced Member

  • Members
  • PipPipPip
  • 756 posts
  • LocationCalifornia

Posted 08 December 2012 - 11:03 AM

What you did wrong, that is easy, you did not test. And not just test, but test at different thicknesses of application and at different cones to see the best results for your work. Do some testing, including a burning off of an application. If the burning off goes well, that is what you can do for the thirty pieces or try applying another coat on top of the first coat, but test.
John 3:16
"For God so loved the world that He gave His only begotten Son, that whosoever believeth in Him should not perish but have everlasting life".

#4 Matt Oz

Matt Oz

    Advanced Member

  • Members
  • PipPipPip
  • 308 posts
  • LocationMichigan

Posted 08 December 2012 - 12:45 PM

Reading this Ducan Overglaze guides Problem section, sounds like it was fired over 018.

Duncan Overglaze.pdf


It says you can burn off the metallic buy firing to 06. Do a test with one of the pots and use witness cones to make sure your firing to 019-018.

Good luck

#5 Marcia Selsor

Marcia Selsor

    Professor Emerita, MSU-Billings

  • Members
  • PipPipPip
  • 5,438 posts
  • LocationBrownsville, Texas

Posted 08 December 2012 - 01:01 PM

If you decide to burn off the metallic lusters, make sure you clean the surface with a luster cleaner or thinner, let it dry before you reapply.

Marcia


Marcia Selsor, Professor Emerita,
Montana State University-Billings

Marcia Selsor Studio in Brownsville, Texas.

http://www.marciaselsorstudio.com


#6 socaljim

socaljim

    Newbie

  • Members
  • Pip
  • 2 posts

Posted 11 December 2012 - 02:32 AM

Thank you all for the advice. Next time I am doing something I have never done before, I will defiantly test before I proceed. Thanks again.