Well, after weeks of acquiring the parts, and piecing the thing together, I finally took my Raku kiln out for a spin.

 

First off, I'd like to thank all those, who helped me through the building process. Your answers are still much appreciated.

My goal was for the thing to just work, and work it did.

The temperature didn't seem to want to come up on a couple occasions, and each time I checked the burner, it turned out that I just didn't have the valve open all the way. The adjustment for the valve, feels springy, so each time I thought it was all the way open, turns out, I could open it a bit more.

The fiber blanket kept the outside of the kiln, as cool as a cucumber...relatively speaking.

 

I was able to fire a medium sized vase, and a test tile for all the available glazes, so my students can get an idea of the colors.

 

A couple issues, one, I have some soot built up on the insulation. I'm guessing this means that I had the burner too close, which didn't allow the propane to completely burn?

Second, some of the glazes turned out kind of "foamy" or "bubbly" looking. Would that mean, that they didn't mature? That is a possibility, but the glazes I used on my vase, turned out fairly glossy.

I couldn't seem to get the temperature much over 1700, though I'm not sure the pyrometer works completely. I tested it in my classroom kiln first, which has a built in pyrometer, and there was a disparity between the two readings.

 

Still, it was a fun experience, despite the worry, that something might go catastrophically wrong. I'm looking forward to trying this with my students.

Share this post


Link to post
Share on other sites

Congratulations! Almost like taking a test drive in a new car without the new car smell.

 

The bubbling means the glaxe never got a chance to completely flow. All raku glazes are not made equal. Make note of those that needed longer firing time and make them your third load and only put in pots using those glazes maturing at a slower pace. If you ever do vessels with narrow necks (like bottles) don't use the bubbling glazes on the inside--they will clog up the necks and even after grinding and refiring, I've never been able to get the glaze to flow. On the outside, grind off the bubbles, reglaze and fire again.

 

Are you able to check the surface of the pots before ending the firing cycle? I never pull pots until they have glossed.

 

The soot usually happens when your oxygen is overpowered by the propane. When it happens, try pulling your burner back away from the burner hole so more air is available to mix with the propane.

 

Shirley

Share this post


Link to post
Share on other sites

Congratulations! Almost like taking a test drive in a new car without the new car smell.

 

The bubbling means the glaxe never got a chance to completely flow. All raku glazes are not made equal. Make note of those that needed longer firing time and make them your third load and only put in pots using those glazes maturing at a slower pace. If you ever do vessels with narrow necks (like bottles) don't use the bubbling glazes on the inside--they will clog up the necks and even after grinding and refiring, I've never been able to get the glaze to flow. On the outside, grind off the bubbles, reglaze and fire again.

 

Are you able to check the surface of the pots before ending the firing cycle? I never pull pots until they have glossed.

 

The soot usually happens when your oxygen is overpowered by the propane. When it happens, try pulling your burner back away from the burner hole so more air is available to mix with the propane.

 

Shirley

 

 

All Raku glazes are not created equal, especially, when mine aren't technically Raku glazes. They are the same low fire glazes I used in my classroom.

Thanks for the tip, regarding the use of bubbling glazes on narrow necks. Honestly, I don't make a lot of vessels like that, but that's probably something I wouldn't even think of.

 

I couldn't really check the pots visually,l despite my best effort. The flame was shooting out the top too much, and I didn't have a ladder tall enough to get far enough away, to avoid the flame. It didn't help that the slight wind kept changing direction, so the flame kept moving.

Some of the glazes did look "wet", when I went to pull them. Oddly enough though, some had brighter, almost ember look spots on the glaze.......unless I'm seeing things.

 

I figured the soot was caused by something like that. I fiddled with the spacing, when the temperature stalled, but pulled it back later.

Share this post


Link to post
Share on other sites

I couldn't really check the pots visually,l despite my best effort. The flame was shooting out the top too much, and I didn't have a ladder tall enough to get far enough away, to avoid the flame. It didn't help that the slight wind kept changing direction, so the flame kept moving.

Some of the glazes did look "wet", when I went to pull them. Oddly enough though, some had brighter, almost ember look spots on the glaze.......unless I'm seeing things.

 

I figured the soot was caused by something like that. I fiddled with the spacing, when the temperature stalled, but pulled it back later.

 

 

If flame was shooting out of the top that intensely, you were almost certainly creating a reduction atmosphere in the kiln. This can not only slow your firing, but create undesirable effects in your glazes (swarms of muddy reds and browns. for instance).

 

Ironically, cranking your burner up too much may create this effect... which actually can slow the firing cycle.

Share this post


Link to post
Share on other sites

I couldn't really check the pots visually,l despite my best effort. The flame was shooting out the top too much, and I didn't have a ladder tall enough to get far enough away, to avoid the flame. It didn't help that the slight wind kept changing direction, so the flame kept moving.

Some of the glazes did look "wet", when I went to pull them. Oddly enough though, some had brighter, almost ember look spots on the glaze.......unless I'm seeing things.

 

I figured the soot was caused by something like that. I fiddled with the spacing, when the temperature stalled, but pulled it back later.

 

 

If flame was shooting out of the top that intensely, you were almost certainly creating a reduction atmosphere in the kiln. This can not only slow your firing, but create undesirable effects in your glazes (swarms of muddy reds and browns. for instance).

 

Ironically, cranking your burner up too much may create this effect... which actually can slow the firing cycle.

 

 

*Shakes fist* Curse you irony!!!

 

So, what would be a better solution? Should I ramp up the temperature more slowly?

Share this post


Link to post
Share on other sites

I couldn't really check the pots visually,l despite my best effort. The flame was shooting out the top too much, and I didn't have a ladder tall enough to get far enough away, to avoid the flame. It didn't help that the slight wind kept changing direction, so the flame kept moving.

Some of the glazes did look "wet", when I went to pull them. Oddly enough though, some had brighter, almost ember look spots on the glaze.......unless I'm seeing things.

 

I figured the soot was caused by something like that. I fiddled with the spacing, when the temperature stalled, but pulled it back later.

 

 

If flame was shooting out of the top that intensely, you were almost certainly creating a reduction atmosphere in the kiln. This can not only slow your firing, but create undesirable effects in your glazes (swarms of muddy reds and browns. for instance).

 

Ironically, cranking your burner up too much may create this effect... which actually can slow the firing cycle.

 

 

 

*Shakes fist* Curse you irony!!!

 

So, what would be a better solution? Should I ramp up the temperature more slowly?

 

 

 

You want to ensure that the oxygen feed is adequate. There are various ways to do this (backing the burner away from the kiln aperture, opening dampers on the kiln- if there are any). However, if you start seeing orange flames shooting out of the top, you'll almost certainly want to back off (slowly) on the burner.

 

It's a finicky process, and can be impacted by things like the ambient temperature/pressure (not to mention the phase of the moon and the number of racoons farting in the nearby shrubbery). However, you do want to avoid an in-kiln reduction atmosphere where possible... both for surface effects and for fluidity of the firing process.

Share this post


Link to post
Share on other sites

I agree with Kohaku. Racoons' farts are a nuisance! Really sometimes it feels like that. As for the burner, you need more secondary air coming through the burner port. Back it out so air can be sucked in with the flame. ou shouldn't need to open it up all the way for gas. Try for an oxidation flame: shorter and harder.

 

Congrats on getting it going. Now it will just need a little tweeking.

 

Marcia

Share this post


Link to post
Share on other sites

you need some kind of peephole or 2, to get a look at the stuff...need a visual on the glaze to get it right imo, too many variables to count on a pyrometer....protect your eyes with some welders glasses too

Share this post


Link to post
Share on other sites

I find a use the pyrometer as much as my peephole, to be honest. I certainly look for that nice 'moonlight on ice' texture with my maturing glossy glazes... but there seems to be a window of temperature between about 1650 and 1850 where the differences in appearance are pretty subtle. I try to go for an even increase to 1850 (unless I'm firing mattes).

Share this post


Link to post
Share on other sites

all true....once you know your glazes and have verified you can probably trust the pyrometer...although, for me, the size of the work makes a big factor in glaze maturation temp

 

i dont actually own a pyrometer, i tune in in the color in the peephole, i dont even look in anymore, a certain shade of orange/yellow and i know i'm there

Share this post


Link to post
Share on other sites

I couldn't really check the pots visually,l despite my best effort. The flame was shooting out the top too much, and I didn't have a ladder tall enough to get far enough away, to avoid the flame. It didn't help that the slight wind kept changing direction, so the flame kept moving.

Some of the glazes did look "wet", when I went to pull them. Oddly enough though, some had brighter, almost ember look spots on the glaze.......unless I'm seeing things.

 

I figured the soot was caused by something like that. I fiddled with the spacing, when the temperature stalled, but pulled it back later.

 

 

If flame was shooting out of the top that intensely, you were almost certainly creating a reduction atmosphere in the kiln. This can not only slow your firing, but create undesirable effects in your glazes (swarms of muddy reds and browns. for instance).

 

Ironically, cranking your burner up too much may create this effect... which actually can slow the firing cycle.

 

 

 

*Shakes fist* Curse you irony!!!

 

So, what would be a better solution? Should I ramp up the temperature more slowly?

 

 

 

You want to ensure that the oxygen feed is adequate. There are various ways to do this (backing the burner away from the kiln aperture, opening dampers on the kiln- if there are any). However, if you start seeing orange flames shooting out of the top, you'll almost certainly want to back off (slowly) on the burner.

 

It's a finicky process, and can be impacted by things like the ambient temperature/pressure (not to mention the phase of the moon and the number of racoons farting in the nearby shrubbery). However, you do want to avoid an in-kiln reduction atmosphere where possible... both for surface effects and for fluidity of the firing process.

 

 

 

I was fairly certain I cleared the area of all raccoons. However, there are plenty of squirrels, and I can't verify their level of gas output.

 

When you say "Back off the burner", do you mean, move it further away from the aperture, to allow more oxygen in, or to turn down the burner?

Share this post


Link to post
Share on other sites

I agree with Kohaku. Racoons' farts are a nuisance! Really sometimes it feels like that. As for the burner, you need more secondary air coming through the burner port. Back it out so air can be sucked in with the flame. ou shouldn't need to open it up all the way for gas. Try for an oxidation flame: shorter and harder.

 

Congrats on getting it going. Now it will just need a little tweeking.

 

Marcia

 

 

You offered quite a bit of help, in my initial stages of building, so thanks again.

Share this post


Link to post
Share on other sites

I couldn't really check the pots visually,l despite my best effort. The flame was shooting out the top too much, and I didn't have a ladder tall enough to get far enough away, to avoid the flame. It didn't help that the slight wind kept changing direction, so the flame kept moving.

Some of the glazes did look "wet", when I went to pull them. Oddly enough though, some had brighter, almost ember look spots on the glaze.......unless I'm seeing things.

 

I figured the soot was caused by something like that. I fiddled with the spacing, when the temperature stalled, but pulled it back later.

 

 

If flame was shooting out of the top that intensely, you were almost certainly creating a reduction atmosphere in the kiln. This can not only slow your firing, but create undesirable effects in your glazes (swarms of muddy reds and browns. for instance).

 

Ironically, cranking your burner up too much may create this effect... which actually can slow the firing cycle.

 

 

 

*Shakes fist* Curse you irony!!!

 

So, what would be a better solution? Should I ramp up the temperature more slowly?

 

 

 

You want to ensure that the oxygen feed is adequate. There are various ways to do this (backing the burner away from the kiln aperture, opening dampers on the kiln- if there are any). However, if you start seeing orange flames shooting out of the top, you'll almost certainly want to back off (slowly) on the burner.

 

It's a finicky process, and can be impacted by things like the ambient temperature/pressure (not to mention the phase of the moon and the number of racoons farting in the nearby shrubbery). However, you do want to avoid an in-kiln reduction atmosphere where possible... both for surface effects and for fluidity of the firing process.

 

 

 

I was fairly certain I cleared the area of all raccoons. However, there are plenty of squirrels, and I can't verify their level of gas output.

 

When you say "Back off the burner", do you mean, move it further away from the aperture, to allow more oxygen in, or to turn down the burner?

 

Back it out of the burner port so it can draw in secondary air for cleaner gas consumption.

Marcia

Share this post


Link to post
Share on other sites

I couldn't really check the pots visually,l despite my best effort. The flame was shooting out the top too much, and I didn't have a ladder tall enough to get far enough away, to avoid the flame. It didn't help that the slight wind kept changing direction, so the flame kept moving.

Some of the glazes did look "wet", when I went to pull them. Oddly enough though, some had brighter, almost ember look spots on the glaze.......unless I'm seeing things.

 

I figured the soot was caused by something like that. I fiddled with the spacing, when the temperature stalled, but pulled it back later.

 

 

If flame was shooting out of the top that intensely, you were almost certainly creating a reduction atmosphere in the kiln. This can not only slow your firing, but create undesirable effects in your glazes (swarms of muddy reds and browns. for instance).

 

Ironically, cranking your burner up too much may create this effect... which actually can slow the firing cycle.

 

 

 

*Shakes fist* Curse you irony!!!

 

So, what would be a better solution? Should I ramp up the temperature more slowly?

 

 

 

You want to ensure that the oxygen feed is adequate. There are various ways to do this (backing the burner away from the kiln aperture, opening dampers on the kiln- if there are any). However, if you start seeing orange flames shooting out of the top, you'll almost certainly want to back off (slowly) on the burner.

 

It's a finicky process, and can be impacted by things like the ambient temperature/pressure (not to mention the phase of the moon and the number of racoons farting in the nearby shrubbery). However, you do want to avoid an in-kiln reduction atmosphere where possible... both for surface effects and for fluidity of the firing process.

 

 

 

I was fairly certain I cleared the area of all raccoons. However, there are plenty of squirrels, and I can't verify their level of gas output.

 

When you say "Back off the burner", do you mean, move it further away from the aperture, to allow more oxygen in, or to turn down the burner?

 

Back it out of the burner port so it can draw in secondary air for cleaner gas consumption.

Marcia

 

 

Can do. The only reason, I moved the burner closer to the aperture, to begin with, was because the temperature plateaued. So my solution was to move the burner closer, and turn up the gas, which apparently, created a reduction atmosphere.

The next time I fire, I will keep the burner further back, and increase the temperature more slowly.

 

Another question. The person I learned Raku firing from, said that once you get the kiln around seven hundred degrees, you should hold that temperature for several minutes. Any idea, why they would say this?

Share this post


Link to post
Share on other sites

That is when the water smoking occurs, i.e. chemical water burns out. Also quartz inversions occur . check those temps.

Racoons fart?

Everyone has a theory.

 

Marcia

 

 

 

 

 

Ah. I knew that was an issue with bisque firing, I never thought, that it would be with the glaze firing as well. Could that be a reason, some of the glazes bubbled, the fact I didn't hold that temperature?

Share this post


Link to post
Share on other sites

Can do. The only reason, I moved the burner closer to the aperture, to begin with, was because the temperature plateaued. So my solution was to move the burner closer, and turn up the gas, which apparently, created a reduction atmosphere.

The next time I fire, I will keep the burner further back, and increase the temperature more slowly.

 

-------------------------------

If there is any difficulty in moving the burner back, another method to increase secondary air is to place a small fan behind the burner, if that is possible. Not too close, as you don't want any dust to blow into the kiln and onto the glazes.

Cheers. Graeme.

Share this post


Link to post
Share on other sites

Can do. The only reason, I moved the burner closer to the aperture, to begin with, was because the temperature plateaued. So my solution was to move the burner closer, and turn up the gas, which apparently, created a reduction atmosphere.

The next time I fire, I will keep the burner further back, and increase the temperature more slowly.

 

-------------------------------

If there is any difficulty in moving the burner back, another method to increase secondary air is to place a small fan behind the burner, if that is possible. Not too close, as you don't want any dust to blow into the kiln and onto the glazes.

Cheers. Graeme.

 

 

There is nothing preventing me from moving my burner back, so that's something I can try. Using a fan, is possible, though I don't have a nearby power source to run it. There wouldn't be an issue with dust, as my kiln shelf sits several inches above the aperture and burner.

Share this post


Link to post
Share on other sites

Another question. The person I learned Raku firing from, said that once you get the kiln around seven hundred degrees, you should hold that temperature for several minutes. Any idea, why they would say this?

 

 

I can't think of any glaze maturation rationale for this. However, a lot of fracturing happens during the early part of the heating cycle. It's particularly easy to blast to a high temperature early on (whereas it's hard to heat too rapidly at high temperatures)... and your more delicate pieces might not be able to take it. I suspect that your instructor wanted to ensure that your work equalized with the temperature in the kiln.

Share this post


Link to post
Share on other sites

I agree with Kohaku about firing faster. I had a wood fired raku kiln that could hit temperature in a few minutes ..after several hours for firing batch after batch.

The coals were well established and it just needed a few pieces of additional wood to melt the glazes.

I glaze a day or more ahead of the firing and if you are going to blast 'em, then preheat the pieces on top of the kiln or in another kiln.

 

Marcia

Share this post


Link to post
Share on other sites

I am a little behind in geting in on this, but I thought relating some recent experience could be of benefit.

 

I fire with a pyrometer and then visually check the melt once I am close. My rule of thumb is to keep the temperature rising at one degree F per second. On a previous firing I had some bubbling, or really more like frothing, left on a couple of pieces when others had reached maturity. The glaze is a clear crackle I use in almost, if not every, raku firing session. This weekend I refired those along with three kiln loads of companions.

 

On my first kiln load I had one piece that still had some bumpiness to the glaze while others were fine, even though I went well over my usual temp, 1850, for this glaze. For my second load I increased the top temp to 1960 and held it a little and made a closer observation at melt. My glazes were very shiny and wet, and the profile was smooth. This was at around 100 degrees F over my "normal" temperature, with a hold. On my third load, I added my pieces from the previous firing, the one with bumpiness from this session, and the remainder of my new pieces. Again I brought the kiln up to 1960, added a hold at top temp, watched the melt and had a perfect firing. Interestingly the previously fired pieces with "defects" melted and went smooth close to the 1850 mark, while the new pieces had to have the higher temperature and a hold. At 1850 they looked like they were covered with foam, but eventually smoothed out when diligence and experience were brought to bear. Upon reflection, I had made a new batch of the clear crackle which has as its majority constituent Gerstley Borate. I had recently bought out the chemical stock of a retiring potter, including the Gerstley Borate I used to batch the clear crackle. That may have been the reason for the odd performance. It may be time to switch to a frit based recipe. Having fired this kiln many times definitely helped me to feel comfortable in changing the variables while looking for a result. You will ge there too.

 

My point for you is that you can refire the pots with the bubbling and it may smooth out the bubbling. Or, it could also be that you are not getting to and staying at the maturing temperature long enough for your glaze to settle. I had all of the isues you had until I got familiar (and comfortable) with my home built raku kiln. When I started firing my own kiln all I had was color and constant checking the melt, but having a pyrometer has been a big plus for me.

 

I am also wondering if your kiln exhaust port may be too small for the fire power of your burner setup. Your burner port could also be small and cause some of these problems you describe. If you have an inch all around your burner at your burner port, then that is probably sufficient. If your exhaust port is a little larger than the burner port that is also probably sufficient. If it is a good bit bigger, you could always use a kiln shelf as a damper. I use part of one as a damper to hold in some heat until I get up above 1000 and then start openiing up the port as I go higher.

 

Hang in there and you will be firing like a pro in no time.

 

John

Share this post


Link to post
Share on other sites

You never did say what you were using for a burner. From the troubles in set up it sounds like you may be using something like a homemade or Weed burner.

 

While you eventually achieve satisfactory results with that grade of burner, I strongly recommend that you use one of the purpose made Raku burners from Ward Burners or ther commercial manufacturer.

 

Commercial burners offer benefits in consistency, control, efficency. Commercail burners normaly provide a ready means of flame chemisty control and and some adjustment of the btu output. I think you will find it desirable if you intend to fire student work.

 

Lockley

Share this post


Link to post
Share on other sites

My intake and exhaust ports are four and five inches respectively. The intake port is an inch larger, than the end of my burner.

 

In regards to the burner, it is a Red Dragon 100 000 BTU weed burner.

Share this post


Link to post
Share on other sites

I completed my second firing today, with my students.

In some ways, this was more successful, in some ways, no so much.

 

The kiln still seemed to take a while to get up to temperature, and even then, it didn't seem to get quite hot enough.

I took the advice, regarding, pulling back the burner, which did help, at least in regards, to reducing the soot issue, I had the first time.

The glazes did look "wet", when I checked them, yet some still had the same "foamy" look to them.

I may enlarge the burner intake on the kiln, to see if that helps, with getting the kiln up to temperature.

 

I did two firings, back to back, and I'd say, the second batch turned out the best.

 

Another interesting point, as the second batch was finishing, the burner shut off. At first, I thought I was out of gas. Then I realized the tank was coated in frost. So it may have froze up?.....

 

Well, I promised my students, we'd do the firing, and I was a man of my word. Now, with that out of the way it's time to perfect my process, so we can do it again, with even better results.

Share this post


Link to post
Share on other sites

Join the conversation

You can post now and register later. If you have an account, sign in now to post with your account.

Guest
Reply to this topic...

×   Pasted as rich text.   Paste as plain text instead

  Only 75 emoji are allowed.

×   Your link has been automatically embedded.   Display as a link instead

×   Your previous content has been restored.   Clear editor

×   You cannot paste images directly. Upload or insert images from URL.

Sign in to follow this  

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.