Hi, have been reading and thinking and still cannot figure out why. I have an Engobe recipe that I have been using as white. Recently I added 2% Chrome Ox to a few hundred grams.

After bisque firing, the colour is a medium sage green. The Clear Satin Glaze shows off the white, but greys out-- almost a blue-grey over the green Engobe. Tthere is no zinc in the clear satin glaze which I otherwise like and use regularly.

 

I want a satin or mat finish, and have no problem testing other glazes, but without understanding if there is something obvious, I don't know where to start.

 

Engobe: EPK 25, Ball Clay 28, NephSy 16, silica 21, Borax 5, Talc 5. Add Bentonite 2, Zircopax 5, Chrome Ox 2

 

Clear Satin Glaze: Gerstley Borate 3, Mag Carb 3, Whiting 23, NephSy 23, EPK 20, Silica 20, 3124 9

 

 

Any insights are very much appreciated.

Thanks

Share this post


Link to post
Share on other sites

First off, satin glazes will always be at least slightly milky, which will affect how clearly the engobe or underglaze underneath shows up. Cobalt can show up blue under a clear glaze, but will go purple as the glaze become more opaque. You may be getting a similar effect here. Second, oxides behave differently underneath a glaze than they do in a glaze. Sorry I can't say anything more specific than that. It could be that you just need more oxide, or try out a different clear.

Share this post


Link to post
Share on other sites
Guest JBaymore

Chromium is affected by the presence of zirconium compounds. Makes it move toward gray tones. You have zirconium in the slip. Add in the fluxing of the overlying glaze and the pickup of both into the boundary layer, and likely that is the culprit. Try the base slip with the chrome but without the zircopax.

 

best,

 

................john

Share this post


Link to post
Share on other sites

Chromium is affected by the presence of zirconium compounds. Makes it move toward gray tones. You have zirconium in the slip. Add in the fluxing of the overlying glaze and the pickup of both into the boundary layer, and likely that is the culprit. Try the base slip with the chrome but without the zircopax.

 

best,

 

................john

 

 

Good to know! I rarely work with chrome.

 

That engobe shouldn't need the zircon anyway. It's plenty opaque as is.

Share this post


Link to post
Share on other sites

Hey, guys;

I avoid chrome as a colourant as it is so flat, like green paint on a fence.

I would suggest using 2% copper carb., and 2% chrome. This will soften it up a bit and give your colour some depth. As always, test,test,test. Right,Neil?

TJR.

Share this post


Link to post
Share on other sites

John, I did wonder about that-- the zircopax and my list of things to try includes making up a new batch of engobe base, now without the zircopax. Working with chrome is new to me but I wanted a green without a bluish hue. I liked the color of the test, and hoped the clear satin would add just enough life to it. Thanks all, fwiw I'll include the results so far, and post the new result when fired.

 

The first time I tested the glaze over engobe, I had granular illmenite in the glaze, so that is what this pic shows. I did another test without the ilemnite, just to make sure it did not cause the color shift. It did not; no difference. Got the same color without the speckles.

post-7168-134922588325_thumb.jpg

post-7168-134922588325_thumb.jpg

Share this post


Link to post
Share on other sites
Guest JBaymore

Chrome oxide is a difficult colorant to use for greens. As TJR said, it generally produces a very "flat" uniform color.... kinda' like paint. Adding a trace of copper or cobalt helps enliven it...... but that is gonna' "shift" it color-wise.

 

best,

 

................john

Share this post


Link to post
Share on other sites

Smartsyartsy;

Actually, Neil is right, you can get very good colour with stains. This is a more expensive way to go.

Don't forget to make a series of tests-probably a line blend to see what percentage of stain you require.

TJR

Share this post


Link to post
Share on other sites

Yes, another option. This piece I am working on is for a dear friend and there is a lot of deep blue glossy glaze (Blueberry). I want the leaves and parts of the background to contrast well. I've got a few options to test-- revise the Engobe, make up a couple of matte glazes, colour a sugary mat I already have,, and may buy a green stain. Everything I am learning here will be of good use for my other botanical tiles.

Share this post


Link to post
Share on other sites

Today's CAD excerpt is about Chrome (John Britt)-- very timely considering I had a very disappointing view of my new chrome tests yesterday. Every one of my tests for adding chrome-- 2 new glaze bases, 2 familiar mat bases--- gave me brownish yuk. The engobe without the zircopax still came out blue/grey under the clear satin glaze.

 

I am digesting this excerpt and looking further into the mystery.

Share this post


Link to post
Share on other sites

i have tried that with mixed results. i have several bowls ready for the 'empty bowl' event our guild supports. i fired two of them that had been covered in a green commercial underglaze, Velvet # 353 and carved. the matt, translucent glaze i sprayed over it made the finished bowl a lovely grey/blue. the very same green used under another glaze is screamingly green, overpowering the other colors i used on that particular bowl.

 

the difference is that the first glaze contains zinc. i have been looking for a great glaze to go over any color and found that zinc is not trustworthy. some colors just fade away when covered with a zinc bearing glaze.

 

i realize that the first post mentioned that there was no zinc in the glaze the poster used. what other ingredients cause the loss of color?

Share this post


Link to post
Share on other sites

oldlady, I have no sure answer for you, but I am still working on solving this problem. I am very curious what glaze went over your third bowl to result in the "screaming green". Would you post the recipe, and I will include it in my test.

Share this post


Link to post
Share on other sites

oldlady, I have no sure answer for you, but I am still working on solving this problem. I am very curious what glaze went over your third bowl to result in the "screaming green". Would you post the recipe, and I will include it in my test.

 

 

 

as j baymore notes below, none of these posts mention a cone number. i work only with cone 6 electric.

 

 

yes, i will send you that glaze. in re-reading the august 30 entry in my notebook, i find it said that the results were "crap", (or just not what i wanted). today, in looking carefully at the finished bowl with the screaming green leaves, i noticed that the soft colors, coral, pink, and purple in the flowers came out fine. the finish is very shiny. it also has unclosed bubbles because my kiln had a broken element. my notes say it was the glaze i got from the mason stain company technician named Vince. he said it would take any of the mason stains but not more than 10%. recipe follows in my format, using the smallest of the ingredients first and working to the most. (have you ever forgotten and left the 1000 gram weight on the scale when making a bucketful af glaze?)

 

EPK 10

whiting 13

silica 325 19

kona f4 26

frit 3124 32 (the actual recommendation was a fusion frit 3292 which i found i could not afford. i was told that 3124 would be close enough.)

 

 

as long as you are testing, and to tease those of you with a great interest in chemical interaction, i will include the following satin matt recipe which has no visible zinc in the list of ingredients but which turns green to grey. a lovely exterior glaze if you are not using green. i would not use it on an interior because of the terrible sound of a metal spoon scraping up the last of something in it.

 

EPK 20

Dolomite 20

Cornwall stone 60

 

i hope this helps, i would love to know your results. i still have 20 bowls due on nov 6. they are all sitting there in the greenware state waiting for me to do them right.

Share this post


Link to post
Share on other sites
Guest JBaymore
i would not use it on an interior because of the terrible sound of a metal spoon scraping up the last of something in it.

 

EPK 20

Dolomite 20

Cornwall stone 60

 

 

What cone is this second glaze intended for?

 

If it is a cone 9 recipe, then there is another potential reason to not use it as a "liner" glaze: it is slightly undersupplied with silica (2.96 mols) for that cone range (which can support up to 5.75 mols). If it is for cone 6, then it is within, but to the low side of usual limits for silica (2.4-4.7 mols).

 

best,

 

.................john

Share this post


Link to post
Share on other sites
Guest JBaymore

sorry, i assumed, (yes, i know!) that all these previous posts were for cone 6 electric, which is all i do.

 

 

No problem whatsoever. I read back through the whole thread and couldn't see a cone range posted anywhere (I still could have missed it :rolleyes: ) ..... which is why I asked.

 

best,

 

................john

Share this post


Link to post
Share on other sites

is anyone working on this? it has been a long time since the last post. now that i have new elements installed (HOORAY< I DID IT!!!) i need to fire those 20 bowls. some have the green underglaze on them and i have covered them in a different glaze this time. if it works, i will share that recipe.

Share this post


Link to post
Share on other sites

SUCCESS!!

 

i am sending out the recipe i found that works to cover amoco velvet green #353 and allows it to remain green. it is from George Wettlaufer's 1976 book, "getting into pots" and he describes it as having a waxy surface. the original recipe called for a feldspar called C-6, a soda spar. when i was unable to find any information on this product (even in the materials list posted on Digitalfire) i called mr. wettlaufer and asked what he would suggest to replace it. his reply was Kona F-4.

 

WETTLAUFER GLAZE 18 CONE 6

 

soda spar (Kona F-4) 40

whiting 15

ball clay, (i use C&C) 20 (i work with white clay so i use the whitest ball clay i can get, C&C but OM4 would work, too)

silica 325 (flint) 15

dolomite 10

 

total 100

 

add 2% bentonite

 

my notes after the first time i used it are VERY NICE SURFACE.

 

this covers colors nicely EXCEPT my mixed underglaze yellow which had floating chunks of yellow suspended above the clay and below the glaze which looked like someone threw yellow sand at a clear paint. unlike other glazes i have tested, this one does not "flatten" texture which is the most important quality for me. if you want to try it, test, test test.

Share this post


Link to post
Share on other sites

csc,

 

have you been trying any of these glazes? i really wish i could send you a picture.

 

i was so pleased that 3 of the green underglazed pieces came out well enough to take to the empty bowl supper on friday. i approached one young man who had one of them and asked why he picked it out of the 400 bowls that were on offer. he said he liked the color. hooray! unfortunately, he dropped it on the driveway as he was leaving. we had some extra bowls and we gave him a green one from another potter so he at least had a green one.

Share this post


Link to post
Share on other sites

I am so glad you found a solution. I am very busy getting glaze firings done for holiday shows. Wll pick up playtime in a couple of months. I wonder if the soda vs potash made the diff. There is also very little magnesium in the "good" glaze.

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now
Sign in to follow this  

×

Important Information

By using this site, you agree to our Terms of Use.