I just fired 2 raku projects.

The first came out all intact and was more slowly fired.

The second, a porcelain paper clay was fired faster had huge cracks in the main body, though the head (a thicker piece) and a hat (thinner lighter )were ok.
Is there a recommended firing schedule and does that change for paper clay?

The instructor does a preheat and then chooses the temp rate to get to cone 06, but if someone knows a recommended schedule for paper clay, I could ask to use that next time.

#2 neilestrick

neilestrick

    Neil Estrick

  • Members
  • PipPipPip
  • 5,051 posts
  • LocationGrayslake, IL

Posted 17 May 2012 - 12:21 PM

I'm thinking the paper pulp had nothing to do with it, but the porcelain body that held the paper did. Porcelain doesn't usually handle the thermal shock of raku firing very well. What clay did you use for the successful piece?

Neil Estrick
Kiln Repair Tech
L&L Kilns Distributor
Owner, Neil Estrick Gallery, LLC
www.neilestrickgallery.com

[email protected]


#3 Marcia Selsor

Marcia Selsor

    Professor Emerita, MSU-Billings

  • Members
  • PipPipPip
  • 6,355 posts
  • LocationRed Lodge, Montana

Posted 17 May 2012 - 03:35 PM

I agree. paper clay isn't the problem, it is the porcelain.
Marcia



Marcia Selsor, Professor Emerita,Montana State University-Billings
[http://www.marciaselsorstudio.com

#4 macdoodle

macdoodle

    Advanced Member

  • Members
  • PipPipPip
  • 84 posts
  • LocationOrange County, CA, USA

Posted 17 May 2012 - 03:39 PM

a-ha, the first was a stoneware.

so porcelain and raku are just a bad combo -and I just got lucky on 2 out of three pieces surviving, THANKS!

maybe my next try i'll do a stoneware paperclay and see what happens :)

#5 Chris Campbell

Chris Campbell

    clay stained since 1988

  • Members
  • PipPipPip
  • 3,117 posts
  • LocationRaleigh, NC

Posted 21 May 2012 - 10:38 AM

I have successfully raku fired porcelain, but it was totally dumb luck ... did not care if it worked, so it did.:P

Paper helps in the pre-firing stages of raw clays by making them stronger and easier to handle and work with ... but it is burned and gone from clay after 451F ... a very low kiln temp. After that you are only dealing with whatever clay body it is. For pit firing and raku, paperclay's benefits lie in the fact that when the paper burns out during bisque, it leaves lovely holes behind to capture glazes and gases.
Chris Campbell Pottery
Contemporary Fine Colored Porcelain
http://ccpottery.com/

>TRY ... FAIL ... LEARN ... REPEAT"

" If a sufficient number of people are different, no one has to be normal "

Fredrick Bachman

#6 JBaymore

JBaymore

    Moderator

  • Moderators
  • 4,271 posts
  • LocationWilton, NH USA

Posted 21 May 2012 - 02:59 PM

If you are going to fire a porcelain clay body as raku (tough to do).... it is best to put them in the first heat-up firing of the kiln, rather than load into a pre-heated kiln. Then bring the kiln up a bit slowly to the maturity of the glazes. When pulled for post firing reduction, smother it in dense combustibles (like sawdust) that retard the cooling, and let it slowly cool right there....... do not water quench it.

As has been said, porcelain does not like thermal shock. The only reason to use a porcelain for raku is the white body background. And that can be accomplished with ANY forumlation of a body that is basically white. It never is getting fired to the vitrifaction point.... that is the whoe rationalle for HAVING porcelain. So try a differnt more thermal shock resistant white-ware body with a buinch of molochite (white) grog in it.

best,

.......................john

John Baymore
Adjunct Professor of Ceramics; New Hampshire Insitute of Art

Former Guest Professor, Wuxi Institute of Arts and Science, Yixing, China

Former President and Past President; Potters Council
 

http://www.JohnBaymore.com

http://www.nhia.edu/...ty/john-baymore


#7 Marcia Selsor

Marcia Selsor

    Professor Emerita, MSU-Billings

  • Members
  • PipPipPip
  • 6,355 posts
  • LocationRed Lodge, Montana

Posted 21 May 2012 - 10:30 PM

I use paper clay in Raku to lighten the weight of my large slabs because they a very heavy at the end of the tongs. some are 25" x 20"and that gets heavy at the end of three foot tongs.
Marcia
Marcia Selsor, Professor Emerita,Montana State University-Billings
[http://www.marciaselsorstudio.com

#8 Chris Campbell

Chris Campbell

    clay stained since 1988

  • Members
  • PipPipPip
  • 3,117 posts
  • LocationRaleigh, NC

Posted 22 May 2012 - 10:20 AM

"The only reason to use a porcelain for raku is the white body background ..."

Well, how about just to see if you can do it? :P
Welcome back to the craziness John!
Chris Campbell Pottery
Contemporary Fine Colored Porcelain
http://ccpottery.com/

>TRY ... FAIL ... LEARN ... REPEAT"

" If a sufficient number of people are different, no one has to be normal "

Fredrick Bachman

#9 Marcia Selsor

Marcia Selsor

    Professor Emerita, MSU-Billings

  • Members
  • PipPipPip
  • 6,355 posts
  • LocationRed Lodge, Montana

Posted 22 May 2012 - 10:54 AM

People do use porcelain for saggar firing in raku kilns but it is a slower firing and lower temperature.
As John says the initial firing would be a good place to try it since that is slow as well. I would also
recommend air cooling after the reduction in a combustion chamber. I would.t dunk it in water. The density is still tight
enough to get shocked.
Marcia
Marcia Selsor, Professor Emerita,Montana State University-Billings
[http://www.marciaselsorstudio.com

#10 JBaymore

JBaymore

    Moderator

  • Moderators
  • 4,271 posts
  • LocationWilton, NH USA

Posted 22 May 2012 - 02:45 PM

"The only reason to use a porcelain for raku is the white body background ..."

Well, how about just to see if you can do it? Posted Image
Welcome back to the craziness John!


Oops... I forgot about the "perverse Don Quixote syndrome" reason. Posted Image

I'm still terribly jetlagged so not really "back"....... coming back to the West from the Far East tends to "peak" about 3-5 days after return........ then it slowly gets better. I'm at the peak time now. Feel like I got hit by a truck Posted Image .

best,

.........................john

John Baymore
Adjunct Professor of Ceramics; New Hampshire Insitute of Art

Former Guest Professor, Wuxi Institute of Arts and Science, Yixing, China

Former President and Past President; Potters Council
 

http://www.JohnBaymore.com

http://www.nhia.edu/...ty/john-baymore


#11 Marcia Selsor

Marcia Selsor

    Professor Emerita, MSU-Billings

  • Members
  • PipPipPip
  • 6,355 posts
  • LocationRed Lodge, Montana

Posted 22 May 2012 - 07:20 PM

John,
Welcome back.Looked like a great show and event.
Congratulations.
Melatonin helps with jet lag.
Marcia


Marcia Selsor, Professor Emerita,Montana State University-Billings
[http://www.marciaselsorstudio.com




0 user(s) are reading this topic

0 members, 0 guests, 0 anonymous users