Here is one posted on Clayart a while back that was taken from lana Wilson's book.

David: I've been using the recipe credited to Lana

Wilson. It turns out white. I subbed OM4 for the

Kentucky ball clay.

 

60 nepheline syenite

22 magnesium carbonate

18 Kentucky ball clay

photo at:

http://www.flickr.com/photos/clayart/1355647449/in/photostream/lightbox/

 

I recommend her book. It is glazing on the Right Side of the brain. Also you could try googling a bead glaze yourself.

Marcia

 

Link to comment
Share on other sites

If you want to purchase these specialty glazes, for the 'crawl glaze' go to http://www.amaco.com...-lead-free.html and for 'Lead Free White Pebble Specialty Glaze SP-400' go to http://www.amaco.com...-lead-free.html . They are both low fire glazes. I am not sure if they can be rakued. You can always ask Amaco if they can be rakued.

Link to comment
Share on other sites

If you want to purchase these specialty glazes, for the 'crawl glaze' go to http://www.amaco.com...-lead-free.html and for 'Lead Free White Pebble Specialty Glaze SP-400' go to http://www.amaco.com...-lead-free.html . They are both low fire glazes. I am not sure if they can be rakued. You can always ask Amaco if they can be rakued.

 

 

 

Here, also is an article on reticulated glazes by R. Hopper.

 

http://ceramicartsdaily.org/ceramic-glaze-recipes/glaze-chemistry-ceramic-glaze-recipes-2/lichens-and-lizards-and-leopards-oh-my-reticulated-glaze-recipes-for-wild-ceramic-surfaces/

 

I do know there are commercial products out there that do a similar thing... ?? Not sure how they would work at Raku temps.

 

Nelly

Link to comment
Share on other sites

Archived

This topic is now archived and is closed to further replies.

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.