After much interest in cooking clay on the stovetop and making BBQs for the yard-I'm posting this for reference . Its the 1973/74 piece from studio potter on flameware and flameware glazes

This is the original clay formula

Ron Propst's Flameware Formula
Spodumene (200 mesh) 30
Pyrophyllite (200 mesh) 10
Feldspar (200 mesh) 10
Ball clay (OM#4) 20
A.P. Green Fireclay 30
Western Bentonite 2
Macaloid

1

The article is here

https://www.studiopotter.org/articles/art0017.htm

you can also google this topic and learn more about flamewares

 

One last thought is flamewars are made to cook on very low heat and very slowly and you run the risk and its always present that the thing will crack and leak . Which can mean burn you or put the stove flame out or spill onto others . So keep this in mind as this clay is very porous and open and will break easy just by hitting or banging it

Edited by Mark C.

Share this post


Link to post
Share on other sites

Create an account or sign in to comment

You need to be a member in order to leave a comment

Create an account

Sign up for a new account in our community. It's easy!

Register a new account

Sign in

Already have an account? Sign in here.

Sign In Now
Sign in to follow this  

×

Important Information

By using this site, you agree to our Terms of Use.