Where Did This Yellowy Colour Come From?


Recommended Posts

Going through my normal glaze frustrations - I added 3.5% titanium dioixde to a paleish grey glaze and it's gone yellowey/ochre colour.

 

Why?

 

I'd expected to get lovely blue/grey with titanium sparkles/slight crystal effect!

 

Clay is a pure white stoneware fired at Orton cone 7 and a half.

 

Recipe is...

 

Soda Feldspar 70

Bentonite 3

Lith Carb 1

Dolomite 7

Zinc Ox 5

Quartz 12

 

Cobalt Ox                .075

Chrome Ox              .075

Nickel Ox                 .05

 

Titanium Dioxide    3.5

 

The rim (which has gone bluey) was dipped again in same glaze + 10% Gillespie Borate.

 

 

post-61816-0-66733400-1494939561_thumb.jpg

post-61816-0-66733400-1494939561_thumb.jpg

Link to comment
Share on other sites

For bluish, I would have tried replacing the titanium with zirconium, of 50/50 zirconium and tin.

 

Yet you may not want to use the tin, as you are including chrome in you glaze. Could cause pink flashing.

 

 

best,

Pres

Link to comment
Share on other sites

Archived

This topic is now archived and is closed to further replies.

×
×
  • Create New...

Important Information

By using this site, you agree to our Terms of Use.