Earthenware bowl
White engobe on alternate facets and on inside
Glaze of 50/50 by weight Cryolite and Nepheline Syenite on outside
Fired to 1050C with 15min soak
Earthenware bowl
White engobe on alternate facets
Glaze of 50/50 by weight Cryolite and Nepheline Syenite on outside
Standard glaze on inside
Fired to 1050C with 15min soak
Earthenware vase, thin walled (approx 2mm thick)
Glaze of 50/50 by weight Cryolite and Nepheline Syenite
Fired to 1050C with 15min soak
Collapsed in kiln